色婷婷丁香六月,钢铁の魔女,久久免费视频7,欧美高清在线视频在线99精品,国产成人精品实拍在线,人人爽人人爽人人片av

Edge Fracture in Mixed Microstructure Steels

2018-12-05 13:26:00
LUQIMENG
Original
2694

Presentation Outline

? Edge Fracture – Background

? Past Case Studies

? Material Evaluations on Production & Trial Material

? Edge quality effects

? Hole expansion testing on current and new grades of AHSS

? Nano-indentation and microstructure

? Concluding Remarks


Edge Fracture – Background

? Fracture initiating at a trimmed edge, typically not predicted by an FLC

? A local formability phenomena: aninter-relationship between steel microstructure, damage during trimming,  and subsequent edge-stretch during forming.

? AHSS more susceptible than single phase materials (Low Carbon, HSLAs)


Edge Fracture – Background

? Edge fractures typically occur in the highest edge strain area in the presence of a rough trimmed edge.

?Typically during drawing or from a stretch flange after a rough die trim.


Edge Fracture Case Studies

? Edge fracture instances are not isolated to particular steel suppliers, grades of AHSS, gauge, or coating.

? Case study subset selected to show common root causes and resolutions.



Front Compartment Rail – CR780T / 420Y (DP).

? This design is frequently used for double attached left / right compartment rails (material utilization)

? Significant edge stretch condition during the draw in the ‘horse collar’ area

? Also, thin bypass condition between common trim lines (difficult to support) affected trim quality.


Rear Rail CR590T / 340YDP

? Intermittent edge fracture predominantly on one hand of part.

?Size and exact location of fractures were variable run-to-run.


Rear Rail CR590T / 340YDP

? LH vs. RH trim conditions made more robust.

? Trim steel insert maintenance required (sharpening).

Potential Sources of Poor Trim Quality

? Poor Nesting (Trimming in Air)

? Die Breathing and Flexing

? Die Guidance

? Improper Clearance

?Typically too tight

?13-15% recommended for most AHSS

? Sharpness of Trim Steels

Part with Flanged Hole – DP980T / 550Y

? Part hole expansion is 13%

? Material capability is 12-15%

? Other material properties within specification

? Hole Expansion (recently added to qualification approval process in May 2014)

? Design not robust for material capability

? Changed material to high yield ratio CR980T / 700Y-MP-LCE

? (HER ~ 30%)

? No issues-to-date


Try-out vs. Production Blanks

? Laser cut blanks in try-out material are not a good indicator of potential edge fractures in production with die struck blanks.

? Stamping plants are concerned about receiving dies for secondary try-out when the dies have not stamped die struck blanks in primary try-out.

? Timing of production-intended blanks needs to ensure that delivery occurs before dies are shipped to home line.


Hole Expansion Testing

? Variability of hole expansion testing exists due to variation in microstructure within a material, the quality of the sheared hole, and specific testing equipment site-to-site.

? A tool for qualification of material and general understanding of edge stretch performance with an adequate sample size; however, challenges exist for use for lot acceptance testing.



Hole Expansion Test

? Mechanical properties of select grades for hole expansion testing.

? Current production DP780 and DP980 vs. newer RA-bearing 1180 MPa grades.

? Mechanical properties of select grades for hole expansion testing.

? Current production DP780 and DP980 vs. newer RA-bearing 1180 MPa grades.


? Newer high strength 1180 MPa grades showing >= HER vs. more conventional DP steels and less sensitivity to edge condition.

? New grades need balance of global and local formability for most applications.

Nano-Indentation Evaluation – DP780

? Nano-indentation testing was performed to determine constituent hardness distributions in mixed microstructure DP780 steel.

? Two production samples were acquired representing two steel sources.

? Under similar blanking and stamping conditions, one steel exhibited edge fracture while the other did not.

? Samples were ground/polished using standard metallurgical techniques and finish-polished with colloidal silica.


? MTS Nanoindenter XP was used.

? Testing was performed at room emperature with a Berkovich tip

? Displacement control was used to indent to 100 nm maximum depth

? 12 x 12 array of indents was placed on each specimen, spaced

2 μm apart ? Resulting hardness was averaged over a 60-90 nm depth to remove any surface abnormalities


Summary

? Edge fracture susceptibility is influenced by a variety of related factors: blank edge condition, material, part design / forming (strain distribution) / trimming process.

? A balance of global and local formability performance is required for most cold-stamped parts and shall be considered in steel development.

? Uniform, fine-grained structure required

? Reduced hardness differential between constituents

? An industry-wide test is needed for material lot acceptance to predict edge fracture susceptibility

? Performance not predicted by standard tensile testing.





Write a Comment
Nine minus Eight =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 丁香花在线观看观看 | 四虎成人免费 | 久青草国产在线 | 国产一级影院 | 成人黄色视屏 | 国产精品一区二区久久精品 | 你懂的国产高清在线播放视频 | 日韩精品午夜视频一区二区三区 | 第四色激情网 | 色女人网站 | 国产成人综合亚洲欧美在 | 丁香六月啪| 久久福利资源国产精品999 | 97在线观看免费观看直播高清 | 嫁给哑巴渔夫 在吃鸡排 | 国内精品一区二区三区 | 国产亚洲网站 | 一级毛片免费毛片一级毛片免费 | 女人30情定水舞间 | 久久77777 | 久久高清一区二区三区 | 男人女人的免费视频网站 | 久久精品人人爽人人爽快 | 黄色视屏免费在线观看 | 国产 欧美 日韩 在线 | 可以免费的视频网站大全 | 婷婷深爱网 | 求av网站 | 久久综合给合久久狠狠狠… | 欧美一区二区三区激情啪啪 | 精品无人区乱码1区2区3区免费 | 国产精品久久久亚洲456 | 精品一区二区三区无卡乱码 | 国产亚洲人成网站在线观看 | 久久成人综合 | 精品久久久中文字幕二区 | 国产色一区 | 四虎影视在线免费观看 | 欧美日韩高清在线观看一区二区 | 四虎影视最新网站在线播放 | 丁香六月在线视频 |